A hardness tester presses an indenter into a material with a set force and turns the depth or the size of the dent into a hardness number on a defined scale, such as HRC, HBW or HV. It is verified in two ways: direct verification checks its forces, its depth or optical measuring system, its test cycle and its indenter, and indirect verification tests certified reference blocks, with a check on a block each day the tester is used.

On this page

What does a hardness tester measure?

Hardness is a material's resistance to permanent deformation by an indenter. NPL points out that it is not an SI quantity. The number comes from a defined test procedure, so it only means something together with its method and scale. The same block gives different numbers on different scales, and converting between them is an approximation.

The common tests differ in the indenter and in what is measured. A Rockwell tester reads depth with its own measuring system. Brinell and Vickers testers measure the size of the indentation optically after the force is removed. A Leeb tester measures a rebound instead of a dent.

The main hardness tests (methods as described by NPL, NIST and Proceq)
TestIndenterWhat is measuredStandards
Rockwell (HR)Diamond cone with a 120° angle and a 0.2 mm tip radius, or a ballThe increase in depth under a two-step forceISO 6508, ASTM E18
Brinell (HBW)BallThe mean diameter of the indentationISO 6506, ASTM E10
Vickers (HV)Square-based diamond pyramid with 136° between opposite facesThe mean length of the two diagonals of the indentationISO 6507, ASTM E92
Leeb (HL)Spring-driven impact body with a hard tipThe rebound velocity divided by the impact velocity, times 1,000ISO 16859, ASTM A956

How a Rockwell tester works

The indenter is brought into contact, a preliminary force is applied and held, and the depth is measured. An additional force then raises the load to the total force, which is held and then taken back to the preliminary force. The depth is measured again, and the hardness comes from the difference h between the two depths (NIST SP 960-5).

On the regular Rockwell scales the preliminary force is 98.07 N (10 kgf) and the total force 588.4 N, 980.7 N or 1471 N (60, 100 or 150 kgf). The superficial scales, for thinner material, use 29.42 N (3 kgf) and 147.1 N, 294.2 N or 441.3 N (15, 30 or 45 kgf).

The hardness number is 100 − h/0.002 mm on the regular diamond scales and 130 − h/0.002 mm on the regular ball scales. The superficial scales use 100 − h/0.001 mm. One regular Rockwell unit is therefore 2 µm of depth and one superficial unit 1 µm, which shows how small the depths are that the tester has to measure.

Common Rockwell scales (NIST SP 960-5, Table 1, with the uses ASTM lists)
ScaleIndenterTotal forceTypical use
HRADiamond cone588.4 N (60 kgf)Cemented carbides, thin steel and shallow case-hardened steel
HRB1.588 mm (1/16 in) ball980.7 N (100 kgf)Copper alloys, soft steels, aluminum alloys and malleable iron
HRCDiamond cone1471 N (150 kgf)Steel, hard cast irons, titanium, deep case-hardened steel and other materials harder than HRB 100
HR15N, HR30N, HR45NDiamond cone147.1 N, 294.2 N or 441.3 NLike the A, C and D scales, for thinner material or case depth
HR15T, HR30T, HR45T1.588 mm (1/16 in) ball147.1 N, 294.2 N or 441.3 NLike the B, F and G scales, for thinner material
Tip: ISO 6508-2:2023 treats tungsten carbide composite balls as the standard Rockwell ball indenter. If an indenter is dropped or knocked, inspect it and verify it again before use, because a diamond can change its performance without visible damage (NIST SP 960-5).

How Brinell and Vickers testers work

A Brinell tester presses a ball into the surface, and after the force is removed the mean diameter of the indentation is measured. NPL gives the usual timing for both Brinell and Vickers: the force is applied over 2 to 8 seconds and held for 10 to 15 seconds. As NPL quotes it, ISO 6506-1 defines HBW = 0.102 × 2F / [πD(D − √(D² − d²))], with the force F in newtons and the ball diameter D and mean indentation diameter d in millimetres.

A Vickers tester uses a square-based diamond pyramid with 136° between opposite faces, and both diagonals of the indentation are measured and averaged. ISO 6507-1 defines HV = 0.102 × 2F sin(136°/2) / d², which works out to about 0.1891 F/d², with F in newtons and the mean diagonal d in millimetres (NPL).

The optical measurement carries a lot of weight. NPL's sensitivity analysis shows that the relative error in HV is twice the relative error in the diagonal, so a 1% error in d gives about a 2% error in HV. The German calibration guideline DKD-R 9-3 limits light-microscope measurement to diagonals of at least 20 µm and calls for a higher-resolution method below that.

Portable testers and the Leeb rebound test

A Leeb tester fires a spring-driven impact body at the surface and measures its speed just before and just after impact. The Leeb hardness is the rebound velocity divided by the impact velocity, times 1,000, so a perfectly elastic rebound would read 1,000 HL (Tietze and Kompatscher, Proceq, IMEKO 2002). The result names the impact device, such as HLD for the standard D device or HLG for the G device used on heavy castings.

ISO 16859-1:2015 covers the test method, ISO 16859-2 the verification and calibration of the devices and ISO 16859-3 the calibration of the reference test blocks. In the US, ASTM A956 covers Leeb testing of steel products. Readings depend on the impact device and the impact direction, and a value converted to HRC or HB depends on the material. The Proceq authors advise treating converted values as informative estimates, not as acceptance values.

Portable Rockwell testers that can meet all the requirements of ASTM E18-25, including direct verification, fall under E18. Portable Rockwell and Brinell testers that can only be verified indirectly fall under ASTM E110.

Direct, indirect and daily verification: what is the difference?

The verification parts of the ISO hardness standards, ISO 6506-2 for Brinell, ISO 6507-2 for Vickers and ISO 6508-2 for Rockwell, specify two methods. Direct verification checks the machine's parts against their tolerances. Indirect verification tests calibrated reference blocks to see how well the machine measures a material of known hardness. ASTM E18-25 covers the same ground for Rockwell in Annex A1, with the standardization of indenters in Annex A3 and of test blocks in Annex A4.

The test method parts add a check the user makes in normal operation. ISO 6508-1:2023 has a normative annex on daily verification (Annex E), and ISO 6507-1:2023 a normative annex on regular checking by the user (Annex C).

The three levels of hardness tester checks
CheckWhat it coversWho and when
Direct verificationThe test forces, the depth-measuring system (Rockwell) or the optical measuring system (Brinell, Vickers), the test cycle and the indenter, each measured with calibrated instrumentsA calibration laboratory or service, at installation, after a rebuild and at the intervals the standard and your procedure set
Indirect verificationThe whole tester on certified reference blocks covering the range of each scale in use, giving its repeatability and its errorA calibration laboratory or service, after direct verification and at regular intervals
Daily or regular checkIndentations on a reference block near the hardness you test, on each scale you will useThe user, before testing on each day of use for Rockwell (ISO 6508-1), and within a week before use, preferably on the day, for Vickers (ISO 6507-1)
Tip: When a tester fails indirect verification, NIST advises using direct verification to find the cause rather than adjusting a component or an electronic offset blindly. Parts that are each within tolerance can still add up to too large an error, and a machine adjusted to offset one error with another may read the blocks well and other materials badly (NIST SP 960-5).

What direct verification checks

The clause titles of ISO 6508-2:2023 show what a direct verification of a Rockwell tester covers: the test force, the depth-measuring system, the test cycle and the machine's hysteresis (clause 5), with the indenters calibrated and verified under clause 7. The Brinell and Vickers parts check the system that measures the indentation instead of the depth system.

  • Test forces. Measured with a calibrated force-measuring instrument. NIST verifies the forces of its own primary hardness machine with load cells (NIST SP 260-269).
  • Depth-measuring system (Rockwell). Checked over its working range. NIST advises resetting any electronic corrections first, so that a correction cannot hide a depth system that is out of tolerance.
  • Optical measuring system (Brinell and Vickers). The system that measures the indentation diameter or diagonals is calibrated (ISO 6506-2:2017 and ISO 6507-2:2018, clause 5.4 in each).
  • Test cycle. The times for applying and holding the force are checked against the standard.
  • Indenter. Diamonds and balls are checked for shape and for performance and come with their own certificates. DKD-R 9-3 recommends recalibrating Rockwell and Vickers indenters, and replacing Brinell balls, 2 years after their first use, with the first-use date written on the indenter's certificate.
  • Hysteresis (Rockwell). Repeated tests with a blunt indenter on a very hard piece should leave no permanent indentation, so any change in the reading comes from the flexing of the machine itself (NIST SP 960-5, ISO 6508-2:2023 clause 5.5).

Indirect verification with reference test blocks

Indirect verification uses certified reference blocks calibrated under ISO 6506-3, ISO 6507-3 or ISO 6508-3, or under ASTM E18 Annex A4 for Rockwell. NIST describes the usual pattern: for each scale, three blocks whose hardness covers the range of the scale, with typically five indentations on each. The range of the readings on a block indicates repeatability, and the difference between their mean and the block's certified value is the error. The limits for both depend on the scale and the hardness level and are tabulated in the standards.

Use the indenter that will be used for testing. NIST also recommends testing one or more blocks as found, before any cleaning, maintenance or adjustment, so the record shows how the tester was performing. If those as-found results are out of tolerance, the hardness tests made since the last verification may be suspect.

Example indirect verification on the HRC scale (illustrative readings)
Certified value of the blockFive readingsMeanRangeError
25.3 HRC25.1, 25.4, 25.0, 25.3, 25.225.20.4−0.1
45.1 HRC45.3, 45.0, 45.4, 45.2, 45.145.20.4+0.1
62.8 HRC62.9, 63.2, 62.8, 63.0, 62.662.90.6+0.1
Tip: Compare each range and error with the limits for your scale and hardness level in the edition of the standard you work to. Record the readings themselves, not only pass or fail.

Where reference blocks get their values

NIST's Rockwell C transfer standards are Standard Reference Materials 2810a, 2811a and 2812a, at nominal 25, 45 and 63 HRC. NIST certified them on its primary hardness standard machine following ASTM E18-25 and ISO 6508-1 to 6508-3, with the forces verified by load cells and the depth system calibrated by laser interferometry against stacks of gauge blocks (NIST SP 260-269, 2026).

Most blocks used in industry are calibrated by secondary calibration laboratories, whose standardizing machines are linked to the national scales (NIST SP 960-5). For the uncertainty of a verification and of measured values, ISO 6508-2:2023 Annex B and ISO 6508-1:2023 Annex G set out the method for Rockwell, and ASTM E18-25 Appendix X2 gives examples.

How to use and look after test blocks

A block's certified value only applies to its top test surface, and each spot can be tested once. NIST's guide gives these practices.

  • Never make an indentation on the bottom of a block. A block that has been tested on the bottom must not be used for verification again.
  • Do not machine a full block to reuse it. The material below the surface may differ, and an indentation deforms material well below it.
  • Spread indentations over the surface rather than filling it from one side, and keep the spacing the standard requires.
  • Clean the block and the anvil, for example with ethyl alcohol, dry them and blow off dust before placing the block.
  • Use the anvil you use for normal testing. On a flat anvil, make one seating indentation first and ignore its value.
  • Keep blocks near the temperature at which they were calibrated. Store them wrapped in anti-corrosion paper rather than oiled, and keep them away from high temperatures, which can age-harden brass blocks.
Tip: NIST notes that the test method standards give typical testing temperatures of 10 °C to 35 °C, and that ISO requires (23 ± 5) °C for tests under controlled conditions.

The daily check before testing

The daily check shows that the tester still reads correctly between verifications. NIST's guide says it should be done at least on each day hardness tests are made, on each scale that will be used, and recommends repeating it whenever the indenter, the anvil or the test force is changed. For Rockwell, ISO 6508-1:2023 requires it before the first test of each day on each scale to be used, and again after the indenter or the test piece support is changed, following the procedure in its Annex E (8.2 and 8.3).

Before the check, make sure the tester moves freely and that the indenter and anvil are seated. After fitting an indenter, make repeated tests on a uniform block until the readings show no rising or falling trend (NIST SP 960-5).

When a tester fails its daily check, the tests made since the last good check may be suspect. NIST highly recommends recording the daily results with statistical process control, such as a control chart, so a drift shows before the tester becomes unacceptable.

How often should a hardness tester be verified?

Each ISO verification part has a clause on the intervals between verifications: clause 7 in ISO 6506-2:2017 and ISO 6507-2:2018, and clause 8 in ISO 6508-2:2023. The ISO 6506-2 abstract notes that the standard states when each type of verification is required. The intervals themselves are in the paid standards.

In Germany, the PTB guideline DKD-R 9-3 (2023) has accredited laboratories carry out direct verification together with indirect verification at installation, after a modification and at least once a year, following the recommendation in the German national annex of the three standards. Its Rockwell section still refers to the 2015 edition of ISO 6508-2. In the UK, UKAS publication LAB 25 requires indirect verification of calibration and testing machines at least once every 12 months (3.2). Accredited testing laboratories also check their machines on reference blocks at the interval the test standard sets, or before use on each day the machine is used if it sets none (8.2).

Verify again after the tester is moved, repaired or adjusted, and shorten the interval for a tester in heavy use or a harsh environment. ILAC-G24:2022 / OIML D 10:2022 lists the factors for setting intervals from your own results.

What the verification record should show

ISO 6508-2:2023 clause 9 and clause 8 of ISO 6506-2:2017 and ISO 6507-2:2018 cover the verification report or calibration certificate. The list below is good practice for your own records rather than a copy of those clauses.

  • The tester's ID, the scales verified and the standard and edition used.
  • The indenters used, with their IDs and certificates.
  • The reference blocks, with their certificate numbers, certified values and due dates.
  • Each reading, the mean, the range and the error for each block, against the limits.
  • The direct verification results for the forces, the depth or optical system and the test cycle, where these were checked.
  • The as-found results before any adjustment and the as-left results after it.
  • The temperature, the date, who did the work and the next due date.

What if a hardness tester fails as found?

Record the as-found results before anyone adjusts the tester. If its error is outside the limit, ISO 9001 clause 7.1.5.2 asks you to determine whether earlier results were adversely affected and to act as needed. Hardness results are often used to accept material, and ASTM E18 calls the Rockwell test satisfactory for acceptance testing of commercial shipments. List the lots tested since the last good check or verification, and compare the size of the error with how close their readings were to the specification limits.

How to run the daily check on a hardness tester, step by step

  1. Check that the tester moves freely and that the indenter and anvil you will use for parts are clean and seated.
  2. For each scale you will use that day, choose a certified reference block close to the hardness you will test and check its certificate.
  3. Clean the block and the anvil, place the block, and on a flat anvil make one seating indentation and ignore it.
  4. Make the check indentations with the same indenter and test cycle you use for parts, keeping the required spacing.
  5. Compare the mean and the range with the block's certified value and the limits in your procedure, and add them to the control chart.
  6. If the check fails, do not test parts. Clean and reseat the indenter and anvil, repeat the check once, and call for verification if it fails again.
  7. Record the result. If the tester failed, review the tests made since the last good check.

How Axiospec helps with hardness testers

Axiospec is calibration management software. It does not verify a hardness tester or decide whether it passes. The limits, the decision rule and the interval stay with you or your calibration provider. Each tester can be an instrument on the register with its verification history, certificates and next due date, and the interval can be set in days, months or years. Indenters can be instruments in their own right, with their certificates and recalibration dates.

Reference test blocks can sit on the register as reference standards with their own certificates and due dates. With a standard such as ISO 9001 or ISO/IEC 17025 selected for the workspace, you pick the block, or a set tracked as one instrument, from the register as the reference standard when you log a verification, and the record keeps the room temperature and humidity. The block's Reverse Traceability card then lists the testers it was used on. One record holds up to 100 named test points, each with a nominal value, a tolerance and the as-found and as-left readings, so each block on each scale can be its own point.

An accepted Fail or Damaged result puts the tester in quarantine. With a standard selected, any approved Fail, Damaged or Pass with an as-found reading out of tolerance needs an impact written, and any not yet written show in Needs attention. The free plan covers up to 50 active instruments. A new workspace starts with a 45-day trial of Professional, with room for 1,500 active instruments and no credit card. We load your existing records for you at no charge on every plan.

Common questions

How do you calibrate a Rockwell hardness tester?
A Rockwell tester is verified directly, by measuring its test forces, depth-measuring system, test cycle and indenter with calibrated instruments, and indirectly, by testing certified reference blocks across the range of each scale. In the indirect verification, the range of the readings on each block shows repeatability and the difference from the certified value shows the error.
What is the difference between direct and indirect verification of a hardness tester?
Direct verification checks the tester's parts against their tolerances, such as the forces, the depth or optical measuring system and the indenter. Indirect verification checks the whole tester by measuring reference blocks of known hardness.
How often should a hardness tester be verified?
The ISO verification standards set the intervals in their own clauses. In Germany, DKD-R 9-3 has accredited laboratories verify directly and indirectly at installation, after a modification and at least once a year. Separately, the user checks the tester on a reference block each day it is used, as NIST SP 960-5 recommends and ISO 6508-1:2023 requires for Rockwell.
How often should you check a hardness tester with a test block?
At least on each day hardness tests are made, on each scale you will use, and again after changing the indenter, the anvil or the test force, as NIST recommends. ISO 6508-1:2023 Annex E gives the daily verification procedure for Rockwell testers.
Can you use both sides of a hardness test block?
No. The certified value applies only to the top test surface, and NIST says a block that has been indented on the bottom must not be used for verification again.
Can Leeb hardness be converted to Rockwell or Brinell?
Conversion tables exist, but the result depends on the material and the impact device. The Proceq authors who described the method advise treating converted values as informative estimates, not as acceptance values.

Put it into practice

Got a gage list? Send it over and we load it for you, usually in a couple of business days. Free on every plan. Then log every calibration to a tamper-evident audit trail and produce records on demand.